# What is chloride stress corrosion cracking?

> Chloride stress corrosion cracking is cracking of stainless steel under tensile stress in water or wet deposits that contain chlorides. Austenitic grades such as 304 and 316 are the most susceptible, duplex grades less so, and risk rises on warm metal. Cracks are fine and branched, with little visible corrosion. API RP 583 covers its external form under insulation.

- Label: Fact
- Type: Explainer
- Published: 2026-11-14T11:53:52+09:00
- By: Jun Zhong
- Researched and drafted by: Beacon's AI newsroom
- Checked by: Jun Zhong on 2026-11-14
- Topics: LNG, Refining, Upstream and offshore
- Canonical: https://beacon.winda.ai/library/chloride-stress-corrosion-cracking/

## Why does it matter?

In October 2013 the UK Health and Safety Executive (HSE) warned that stainless steel thermowells on a refinery reactor had cracked from the inside [1]. Each time the reactor cooled, the tubes pulled in outside air carrying halides from the coastal or cooling tower atmosphere, and the salts built up in internal crevices until cracks started [1]. Some cracks lay below the reactor flange, where a through-wall crack would have released hazardous material [1]. In 2015 the HSE reported the same mechanism offshore in stainless pipe connectors, and noted that radiography showed internal cracks that visual and dye penetrant checks had not revealed [2].

## How does chloride stress corrosion cracking happen?

Like other stress corrosion cracking, it needs a susceptible alloy, an aggressive environment and enough tensile stress at once; remove any one and it does not occur [10]. Here the environment is water or a moist salt film containing chloride ions, and the stress can be applied load or residual stress from welding or forming [4][5]. The connector cases show that the stress need not come from process pressure: the swaged driver ring holds a permanent hoop stress [2].

Cracks grow with very little general corrosion around them [10]. In cross-section they branch repeatedly, a pattern failure analysts use to identify stress corrosion cracking [5]. In austenitic stainless steel the cracks run mostly through the grains (transgranular), with some branches along grain boundaries; in steel already sensitized by heat, the path is often along the boundaries (intergranular) [4][7].

## Which alloys are most susceptible?

- **Standard austenitic grades.** Resistance depends on nickel content, and grades with about 8 to 10% nickel by weight, which include 304/304L and 316/316L, are the most susceptible [3]. In US Nuclear Regulatory Commission (NRC) salt fog tests at 43 °C (109 °F), 304 and 304L specimens showed attack after 4 weeks and 316L after 32 weeks [4].
- **High-alloy austenitic grades.** More nickel and molybdenum, as in 6% molybdenum super austenitic steels, gives much better resistance [3].
- **Duplex stainless steels.** Their mixed austenite and ferrite structure places them between the austenitic and ferritic families [3]. They are not immune, and API RP 583 covers both families under insulation [9].
- **Ferritic stainless steels.** Grades such as 430 and 444 are very resistant [3].

No stainless steel grade is completely immune [3].

## What conditions drive it?

- **Temperature.** With the steel fully immersed, cracking below about 60 °C (about 140 °F) is rare [3]. Concentrated salt deposits crack it at lower temperatures: the NRC tests produced cracks at 43 °C but none at 85 or 120 °C, where deposited salt could not absorb enough moisture to form a liquid film [3][4].
- **Chloride concentration and evaporation.** Failures have been reported with as little as 10 ppm chloride in the bulk water where wetting and drying, or a film on a hot surface, concentrated it [3].
- **Oxygen and acidity.** Lower pH raises susceptibility; with very little dissolved oxygen, water with low to moderate chloride rarely cracks 304L or 316L [3].
- **Stress.** Higher tensile stress increases the risk, and in the NRC tests the cracks in welded specimens gathered in the heat-affected zone [3][4].

## Where does it occur in oil and gas facilities?

- **Under insulation.** Wet insulation can leach chlorides onto hot stainless steel, as the National Aeronautics and Space Administration (NASA) describes on steam and condensate lines; a 2022 review notes that stainless steel under insulation suffers mainly pitting and cracking [5][6].
- **Small parts in marine or cooling tower air.** Thermowells and swaged connectors exposed to coastal air or saltwater deluge water have cracked [1][2].
- **Process heaters.** Stainless heater tubes in heavy crude service have failed by intergranular cracking attributed to chlorides in the crude, at about 130 to 345 °C [7].
- **Shutdown washing.** Alkaline washes used against polythionic acid cracking can themselves cause chloride cracking if the wash water or ammonium chloride salts bring chlorides; an industry Q&A describes capping chloride in the wash and adding a sodium nitrate inhibitor for this reason [8].
- **Sour offshore wells.** US rules for offshore hydrogen sulfide zones require materials that resist chloride stress cracking, among other failure modes (30 CFR 250.490(p)) [11].

## How is it found and controlled?

Surface methods find only cracks that break the surface: on the offshore connectors, visual and dye penetrant inspection missed internal cracks that radiography revealed [2]. In the refinery, one visible crack on a thermowell extension led to full-length examination of the others, which showed cracks growing from the inside [1]. Confirming the mechanism usually needs a metallographic section showing the branched crack path [4][5].

Control measures in public sources include a more resistant alloy, dry insulation behind intact jacketing, low-chloride insulation, coatings under insulation and lower residual stress [3][5][6]. HSE notes that paint may not remove the risk on connectors, because a crevice can still start localized corrosion [2]. For thermowells, HSE asked operators to register those whose failure could release hazardous substances and to plan inspection accordingly [1].

## Where integrity problems show up

| Where it occurs (unit or equipment) | Conditions that drive it | How it is usually found | In the Library |
|---|---|---|---|
| Insulated stainless steam, condensate and process lines | Wet insulation leaching chlorides onto hot metal [5][6] | Branched cracks confirmed in failure analysis sections [5] | [What is corrosion under insulation (CUI)?](/library/corrosion-under-insulation/) |
| Stainless thermowells on reactors near the coast or cooling towers | Halide-laden air drawn in as the thermowell heats and cools; salts concentrate in crevices [1] | A visible crack during routine maintenance, then full-length examination of the other thermowells [1] | [What are the main non-destructive testing (NDT) methods in oil and gas?](/library/ndt-methods-overview/) |
| Swaged 316/316L pipe connectors offshore | Permanent hoop stress in the driver ring; marine air or saltwater deluge [2] | Radiography found internal cracks that visual and dye penetrant inspection missed [2] | [Radiographic testing](/glossary/radiographic-testing/) |
| Stainless heater tubes in heavy crude service | Chlorides in the crude at about 130 to 345 °C [7] | Failure analysis showed intergranular cracking [7] | [What is a fired heater?](/library/fired-heater/) |
| Welded stainless equipment in marine air | Sea salt deposits that absorb moisture just above ambient temperature; weld residual stress [4] | Metallographic sections; in NRC tests, cracks gathered in the heat-affected zone [4] | [What is atmospheric corrosion?](/library/atmospheric-corrosion/) |

Sources: HSE safety alerts HID 2-2013 [1] and ED 01-2015 [2]; NRC NUREG/CR-7030, 2010 [4]; NASA KSC [5]; Cao and others, 2022 [6]; Ardila-Parra and others, 2026 [7].

## Sources

1. [Safety alert HID 2-2013: Chloride induced stress corrosion cracking of stainless steel thermowells: potential for ingress of atmospheric moisture, UK Health and Safety Executive (HSE)](https://www.hse.gov.uk/safetybulletins/thermowell-corrosion.htm), 2013-10-08
2. [Safety alert ED 01-2015: External chloride stress corrosion cracking of stainless steel Lokring pipe connectors, UK Health and Safety Executive (HSE)](https://www.hse.gov.uk/safetybulletins/lokring-pipe-connectors.html), 2015-04-14
3. [Chloride Stress Corrosion Cracking, Specialty Steel Industry of North America (SSINA)](https://www.ssina.com/education/corrosion/chloride-stress-corrosion-cracking/), 2019-08-20
4. [NUREG/CR-7030, Atmospheric Stress Corrosion Cracking Susceptibility of Welded and Unwelded 304, 304L, and 316L Austenitic Stainless Steels Commonly Used for Dry Cask Storage Containers Exposed to Marine Environments (L. Caseres, T. S. Mintz), US Nuclear Regulatory Commission (NRC)](https://www.nrc.gov/regulations-legislation/nureg-series-publications/publications-prepared-by-nrc-contractors/cr7030)
5. [Forms of Corrosion, NASA Kennedy Space Center (KSC), Corrosion website](https://public.ksc.nasa.gov/corrosion/forms-of-corrosion/)
6. [A Review of Corrosion under Insulation: A Critical Issue in the Oil and Gas Industry (Q. Cao and others), Metals 12(4):561, MDPI (open access, CC BY)](https://doi.org/10.3390/met12040561)
7. [Understanding failure in austenitic steels: Key considerations for molten salt storage in CSP applications (S. A. Ardila-Parra, C. Prieto, J. D. Osorio, A. I. Fernández), Journal of Materials Research and Technology 41, US Department of Energy, Office of Scientific and Technical Information (OSTI)](https://www.osti.gov/servlets/purl/3027701)
8. [Q&A, Question 20: When is it appropriate to neutralize austenitic stainless-steel equipment to protect against stress corrosion cracking?, American Fuel & Petrochemical Manufacturers (AFPM)](https://afpm.org/print/pdf/node/42154)
9. [2025 Publications Catalog (entries for RP 583 and RP 571) (RP 583, 2nd edition, March 2021; RP 571, 3rd edition, March 2020), American Petroleum Institute (API)](https://www.api.org/-/media/files/publications/2025-catalog/2025_pubs%20catalog.pdf)
10. [NIST Special Publication 780, Guidelines for Pressure Vessel Safety Assessment (S. Yukawa), US National Institute of Standards and Technology (NIST)](https://nvlpubs.nist.gov/nistpubs/Legacy/SP/nistspecialpublication780.pdf)
11. [30 CFR 250.490, Hydrogen sulfide, Electronic Code of Federal Regulations (eCFR)](https://www.ecfr.gov/current/title-30/section-250.490)
12. [Stress Corrosion Cracking: Case Studies in Refinery Equipment (G. R. Lobley), 6th Saudi Engineering Conference, Vol. 5, King Fahd University of Petroleum and Minerals (KFUPM), conference proceedings](https://faculty.kfupm.edu.sa/coe/sadiq/proceedings/SEC2002/vol5/P017.pdf)