# What is metal dusting?

> Metal dusting is severe high-temperature corrosion in which iron-, nickel- and cobalt-based alloys break down into a dust of metal, carbon and oxides. It occurs in carbon-rich gases, typically between about 400 and 800 °C, and causes deep pits and heavy metal loss, mainly in hydrogen, syngas, ammonia and methanol plants.

- Label: Fact
- Type: Explainer
- Published: 2026-11-14T12:02:06+09:00
- By: Jun Zhong
- Researched and drafted by: Beacon's AI newsroom
- Checked by: Jun Zhong on 2026-11-14
- Topics: LNG, Refining
- Canonical: https://beacon.winda.ai/library/metal-dusting/

## Why does it matter?

Metal dusting attacks the stainless steels and nickel alloys chosen for hot, carbon-rich service, not only carbon steel: a 2002 study notes that iron, nickel and cobalt, and the alloys based on them, are all susceptible [3]. Avoiding it has shaped plant design. A US Department of Energy (DOE) fact sheet notes that reformer plants have long quenched hot process gas with water from about 800 to 400 °C (about 1,470 to 750 °F) to avoid metal dusting attack, giving up high-grade heat [1]. A 2011 review describes the outcome of metal dusting as severe metal loss from process units, with costly maintenance and serious safety issues [4].

## How does metal dusting happen?

It needs a gas that is supersaturated in carbon, meaning its carbon activity is above 1, such as mixtures of carbon monoxide and hydrogen [3][5]. Sources give the damaging temperature range as about 400 to 800 °C (about 750 to 1,470 °F) [1][5], or 300 to 850 °C in one study of pure metals [3].

In iron and steel, carbon collects at the surface and forms an unstable iron carbide, which then breaks down as graphite grows into it; iron atoms migrate into the graphite and are carried off as fine particles [3]. Nickel and cobalt form no such carbide, so their atoms pass into the graphite directly [3]. What is left is a deposit of carbon holding metal particles, carbides and oxides [5].

Alloys resist only while a protective oxide scale stays intact. Researchers at Argonne National Laboratory (ANL) found chromium oxide the most protective scale in a reformer environment, while iron-rich spinel oxides could be reduced by carbon [1]. Attack starts where the oxide breaks down and grows as pits [1][3].

## Where does it occur?

- **Hydrogen, ammonia, methanol and syngas production.** DOE lists hydrogen production, ammonia synthesis, methanol reforming and syngas production, as well as catalyst regeneration units in the chemical and petroleum industries [2].
- **Heat recovery equipment.** ANL names waste heat boilers and gas bypass lines in methanol and ammonia reformer plants, along with gas-to-liquids plants [1].
- **Steam reforming in general.** The 2011 review calls steam reforming the setting where metal dusting is most often met [4].
- **Coked furnace coils.** Coke on the inner walls of cracking furnace coils favors carburization and metal dusting at service temperatures [6].

## What reduces it?

- **Alloy chemistry.** ANL developed alloys that form a chromium oxide scale; in a laboratory test they stayed smooth for 5,700 hours, while commercial alloys in the same environment developed large pits [1].
- **Water vapor and temperature.** In tests at Oak Ridge National Laboratory (ORNL), raising the temperature from 550 to 750 °C generally reduced attack in one gas mixture, and adding water vapor at 650 °C reduced it too; the more highly alloyed specimens kept a thin protective oxide for 5,000 hours at 9.1 atmospheres with 20% water vapor [5].
- **Coatings and surface treatments.** A 2011 review covered protective coatings alongside ways of changing the surface itself: adding elements that poison the carburizing reaction, alloying the surface layer, and treating it chemically, mechanically or by laser [4].
- **Process design.** Quenching hot gas through the damaging range avoids it, at a cost in recovered heat [1].

Laboratory rankings need care. With little or no water vapor, ORNL found iron-base alloys less resistant than nickel-base alloys, but the authors note that plant gases can contain up to 40% water vapor at high pressure, and that one plant study reported better results for iron-base alloys [5].

## How is metal dusting found?

The sources reviewed for this page describe metal dusting by the damage it leaves, local pits and metal loss under carbon-rich deposits, rather than by a dedicated field inspection method [1][5]. In the laboratory, ANL used Raman spectroscopy to tell protective from unprotective oxide scales [1]. ORNL notes that a lack of attack in short tests may only reflect the time attack takes to start [5]. Pits and wall loss are forms of local metal loss; for the methods used to find those, see [What are the main non-destructive testing (NDT) methods in oil and gas?](/library/ndt-methods-overview/).

## Where integrity problems show up

| Where it occurs (unit or equipment) | Conditions that drive it | How it is usually found | In the Library |
|---|---|---|---|
| Hydrogen and syngas plant reformer outlet systems, waste heat boilers and gas bypass lines | Carbon-rich gas held or cooled through about 400 to 800 °C [1][2] | As local pits and metal loss on exposed surfaces; no dedicated field method in the sources reviewed [1] | [What are the main non-destructive testing (NDT) methods in oil and gas?](/library/ndt-methods-overview/) |
| Ammonia and methanol reformer plants | Same hot, carbon-rich gas service [1][2] | Seen as pitting and mass wastage of alloy components [1] | [Metal loss](/glossary/metal-loss/) |
| Cracking furnace coils with coke | Coke on inner walls at high service temperatures [6] | Metallography of tubes removed after service [6] | [What is a petrochemical plant?](/library/petrochemical-plant/) |
| Alloys whose chromium oxide scale fails | Iron-rich oxides reduced by carbon; scale defects [1][5] | Laboratory exposure tests with pit measurement and oxide analysis [1][5] | [What is carburization?](/library/carburization/) |

Sources: DOE fact sheets on ANL work [1][2]; ORNL, 2015 [5]; Orlikowski and others, 2021 [6].

## Sources

1. [Argonne National Laboratory Develops Alloys to Resist Metal Dusting (fact sheet), US Department of Energy, Industrial Technologies Program](https://www1.eere.energy.gov/manufacturing/industries_technologies/imf/pdfs/metaldusting.pdf)
2. [Development of Materials Resistant to Metal Dusting Degradation (project fact sheet), US Department of Energy, Industrial Technologies Program](https://www1.eere.energy.gov/manufacturing/industries_technologies/imf/pdfs/16944_metal_dusting.pdf)
3. [On the Mechanism of Metal Dusting Corrosion (C. M. Chun, J. D. Mumford, T. A. Ramanarayanan), meeting abstract 1111, The Electrochemical Society, 201st Meeting](https://www.electrochem.org/dl/ma/201/pdfs/1111.pdf)
4. [Metal Dusting Protective Coatings. A Literature Review (A. Agüero and others), Oxidation of Metals 76: 23-42 (repository record and abstract), INTA (Spanish National Institute for Aerospace Technology) institutional repository](https://digital.inta.es/entities/publication/745707a8-e334-4d89-b9f4-b41d72c1dbcc/full), 2011-03-20
5. [Performance of Chromia- and Alumina-Forming Fe- and Ni-base Alloys Exposed to Metal Dusting Environments: The Effect of Water Vapor and Temperature (A. Rouaix-Vande Put, K. A. Unocic, M. P. Brady, B. A. Pint), Corrosion Science 92, Oak Ridge National Laboratory, via US DOE Office of Scientific and Technical Information (OSTI)](https://www.osti.gov/biblio/1265502)
6. [Investigation of the 0.4C-35Cr-45Ni-Nb Alloy after Service in High-Temperature Steam and Hydrocarbons Environment (J. Orlikowski and others), Materials 14(20):6139, MDPI, via PubMed Central (open access, CC BY 4.0)](https://pmc.ncbi.nlm.nih.gov/articles/PMC8541315/), 2021-10-15

Published by Winda Beacon (https://beacon.winda.ai).