> Polythionic acid stress corrosion cracking is intergranular cracking of sensitized austenitic stainless steels and other austenitic alloys. It typically occurs in refinery units handling sulfur-bearing streams, during shutdowns, when sulfide scale reacts with air and moisture to form polythionic acids that attack chromium-poor grain boundaries under stress. NACE RP0170 covers protection during shutdowns.

- Label: Fact
- Type: Explainer
- Published: 2026-11-13T09:44:04+09:00
- By: Jun Zhong
- Researched and drafted by: Beacon's AI newsroom
- Checked by: Jun Zhong on 2026-11-13
- Topics: Refining
- Canonical: https://beacon.winda.ai/library/polythionic-acid-scc/

## Why does it matter?

Polythionic acid stress corrosion cracking (PTA SCC, also written PASCC) strikes during shutdowns, not in operation [1][3]. A 2002 case study described the stainless steel heater coil of a naphtha hydrotreater that had been shut down and restarted several times over about 18 years, then was found extensively cracked after one shutdown; the alkaline neutralizing wash had not been documented or followed properly, and its protective film had been rinsed off with water [1]. A 2011 failure analysis of stabilized 347 furnace tubes in a hydrocracker, which failed after a shutdown at nearly 8 years, also pointed to errors in the shutdown procedure [2].

## How does polythionic acid cracking happen?

Three things must meet: a sulfide scale, a sensitized austenitic alloy under tensile stress, and air plus moisture [1][3].

1. **In operation, scale forms and the metal may sensitize.** Hydroprocessing units run without oxygen, which favors iron and other metal sulfide scales on hot surfaces [3]. Long exposure to heat forms chromium carbides at grain boundaries and leaves the zones beside them short of chromium (sensitization) [3][6].
2. **At shutdown, acids form.** When equipment is opened, oxygen enters with air, and moisture comes from humidity, washing or steaming out; together they turn the sulfide scale into polythionic acids, a family of sulfur acids written H2SxOy [1][3].
3. **Under stress, cracks follow the grain boundaries.** The acids dissolve the chromium-poor zones, and laboratory work with a tetrathionate solution showed the crack tip advancing along grain boundaries as load was applied, so stress matters as well as dissolution [4].

Researchers have debated which sulfur acid does the damage: early work in the 1960s pointed to polythionic acids, another view to sulfurous acid, and a 1984 study to tetrathionic acid as the only one of them that cracks sensitized 304 [1].

## Which equipment and materials are susceptible?

- **Sensitized austenitic alloys.** The cracking affects sensitized austenitic stainless steels and other austenitic alloys [3]. How much sensitization and stress it takes is not well understood; sensitization proceeds faster at higher temperature and depends on composition [3].
- **Hydroprocessing units.** Reactor circuit sections often operate in the sensitizing range, and stainless heater tubes can be attacked on both inside and outside surfaces [3].
- **Equipment hotter than the process.** In the 2002 case the process stream was 330 °C, which seemed too cool to sensitize the coil, but tube metal temperature in the fired heater was about 405 °C [1]. Early researchers thought service below 800 °F (427 °C) would not sensitize these steels, yet a 304 flange in a hydrodesulfurizer cracked after about 15.75 years at up to 384 °C [1].
- **Stabilized grades under local overheating.** Grades stabilized with titanium or niobium, such as 347, resist sensitization [3], but the hydrocracker's 347 tubes sensitized where carbon deposits caused local overheating, which a 2026 review puts at 512 °C [2][5].

## How is it found?

- **At shutdown, by examination.** The hydrotreater coil cracks were found after the unit was shut down, as transverse cracks, some wide open [1]; the hydrocracker tubes showed circumferential cracks beneath carbon deposits [2].
- **In the laboratory, by confirming the path and the cause.** Sections showed cracks starting on the process side and running between grains with some branching; an oxalic acid etch revealed widened grain boundaries typical of sensitized steel, and the inside deposit was about 80% iron sulfide [1]. In the 347 case, microstructure and a double-loop electrochemical potentiokinetic reactivation (DL-EPR) test confirmed sensitization [2].

## How is it prevented during shutdowns?

Measures described in refinery practice include [3][1]:

- **Neutralizing.** Washing equipment with a soda ash solution before it is exposed to air neutralizes acids and leaves a thin alkaline film; every internal surface must be wetted, and the film reapplied if rain, water washing or mechanical work removes it [3]. NACE RP0170 describes soda ash washing and nitrogen purging [1].
- **Keeping air out.** Equipment that will not be opened can be held under nitrogen, though users have found commercial nitrogen carrying far more oxygen than expected [3].
- **Keeping water out.** Dried air with a dew point well below the metal temperature can be used, and heater fireboxes can be kept warm with pilots or a portable heater to protect the outside of stainless tubes [3].
- **Choosing and treating material.** Stabilized grades, a stabilization heat treatment, and heat treatment after forming improve resistance [1][3].

Washing carries its own risk: chlorides in wash water or ammonium chloride salts can cause chloride stress corrosion cracking, so practice includes an inhibitor, a chloride cap, a thorough rinse and drained low points [3].

## Where integrity problems show up

| Where it occurs (unit or equipment) | Conditions that drive it | How it is usually found | In the Library |
|---|---|---|---|
| Type 304 charge heater coils in naphtha hydrotreaters | Tube metal about 75 °C hotter than the process; sulfide scale; neutralizing film rinsed off at shutdown [1] | Cracks seen after shutdown; metallography and etching confirmed intergranular cracking in sensitized steel [1] | What is a fired heater? |
| Type 347 furnace tubes in hydrocracker fractionators | Local overheating under carbon deposits; errors in shutdown procedure [2][5] | Circumferential cracks under deposits after shutdown; microstructure and DL-EPR confirmed sensitization [2] | [What is hydroprocessing (hydrotreating and hydrocracking)?](/library/hydroprocessing/) |
| Hydroprocessing reactor circuits and heater tubes, inside and outside | Sulfide scale from oxygen-free operation; air and water when opened [3] | Risk mapped before the shutdown by identifying where scale and susceptible alloy meet [3] | How is inspection scope set for a turnaround? |

Sources: Lobley, 2002 [1]; Swaminathan and others, 2011 [2]; AFPM, 2016 [3]; Ardila-Parra and others, 2026 [5].

## Sources

1. [Stress Corrosion Cracking: Case Studies in Refinery Equipment (G. R. Lobley), 6th Saudi Engineering Conference, Vol. 5, King Fahd University of Petroleum and Minerals (KFUPM), conference proceedings](https://faculty.kfupm.edu.sa/coe/sadiq/proceedings/SEC2002/vol5/P017.pdf)
2. [Sensitization induced stress corrosion failure of AISI 347 stainless steel fractionator furnace tubes (J. Swaminathan, R. Singh, M. K. Gunjan, B. Mahato), Engineering Failure Analysis 18(8), CSIR-National Metallurgical Laboratory (NML), Eprints@NML (abstract)](https://eprints.nmlindia.org/4222)
3. [Q&A, Question 20: When is it appropriate to neutralize austenitic stainless-steel equipment to protect against stress corrosion cracking?, American Fuel & Petrochemical Manufacturers (AFPM)](https://afpm.org/print/pdf/node/42154)
4. [On the mechanism of intergranular stress corrosion cracking of sensitized stainless steel in tetrathionate solution (A. Yonezu, R. Kusano, X. Chen), Journal of Materials Science 48(6):2447-2453, Lingnan University research repository (abstract)](https://scholars.ln.edu.hk/en/publications/on-the-mechanism-of-intergranular-stress-corrosion-cracking-of-se/)
5. [Understanding failure in austenitic steels: Key considerations for molten salt storage in CSP applications (S. A. Ardila-Parra, C. Prieto, J. D. Osorio, A. I. Fernández), Journal of Materials Research and Technology 41, US Department of Energy, Office of Scientific and Technical Information (OSTI)](https://www.osti.gov/servlets/purl/3027701)
6. [Intergranular Corrosion, Association for Materials Protection and Performance (AMPP)](https://ampp.org/technical-research/impact/intergranular-corrosion)