# Sacrificial anode vs impressed current cathodic protection

> Both systems make the protected steel the cathode of a circuit, nearly stopping its corrosion; they differ in the current source. Sacrificial (galvanic) anodes of magnesium, aluminum or zinc corrode instead and need no power. Impressed current uses a rectifier to drive larger, adjustable current. US pipeline criteria for both are in 49 CFR 192 Appendix D.

- Label: Fact
- Type: Explainer
- Published: 2026-11-13T09:44:04+09:00
- By: Jun Zhong
- Researched and drafted by: Beacon's AI newsroom
- Checked by: Jun Zhong on 2026-11-13
- Topics: Pipelines, Upstream and offshore
- Canonical: https://beacon.winda.ai/library/sacrificial-vs-impressed-current/

## Why does it matter?

On December 11, 2012, a 20-inch natural gas transmission line ruptured and burned beside Interstate 77 at Sissonville, West Virginia, destroying three houses [8]. The line had a factory-applied coating and impressed current cathodic protection, and readings at the nearest test station, about 100 feet away, had been satisfactory for 10 years [8]. Yet more than 30 square feet of pipe was heavily corroded, with over 70% wall loss, because coarse rock backfill had damaged the coating and blocked the protective current [8]. Whichever system supplies it, the current protects only steel it can reach [8].

## Sacrificial anode vs impressed current at a glance

| | Sacrificial (galvanic) anodes | Impressed current |
|---|---|---|
| Source of current | The natural voltage difference between a more active metal and the steel [1][3] | An external direct current supply, usually a transformer-rectifier fed from the power grid [1][3] |
| Anode materials | Magnesium, aluminum or zinc alloys cast around a steel insert [1] | Low-dissolution anodes: high-silicon cast iron, graphite, mixed metal oxide on titanium, magnetite; scrap steel as a consumable option [1][2] |
| Driving voltage | About 0.5 V for aluminum and zinc, falling to about 0.25 V as the steel polarizes; up to about 1 V for magnesium [1] | Up to about 50 V [1][2] |
| Current output | Small, governed by soil or water resistivity, not normally adjustable [1] | Large and adjustable as the structure changes [1] |
| Reach on a pipeline | "Little and often": NPL gives about 200 m average spacing for magnesium anodes on a well-coated 300 mm pipe, for 8 to 10 years of anode life [2] | About 2 km per installation on poorly coated pipe, 50 km or more on well-coated pipe [2] |
| Power needed | None [1] | Grid power, or solar, wind, thermoelectric or engine-driven generation in remote areas [1] |
| Effect on nearby structures | Less prone to severe interference, so often used in congested or built-up areas [1][2] | Must be designed to limit stray current effects on neighboring structures [1][5] |
| Overprotection | Generally self-regulating [1] | Excessive negative potentials can disbond coatings and embrittle high-strength steels [1] |
| Routine US pipeline checks | Cathodic protection test every calendar year, no more than 15 months apart [5][7] | The annual test plus rectifier checks six times a year, no more than 2½ months apart [5][7] |
| US Army selection rule (1985) | Soil resistivity below 5,000 ohm-cm (50 ohm-m) and current demand below 1 milliampere per square foot [3] | Resistivity or current demand above those values [3] |

Sources: NPL Guides No. 1 and 4 [1][2]; US Army TM 5-811-7, 1985 [3]; 49 CFR 192.465 and 195.573 [5][7].

## When are sacrificial anodes used?

- **Small or well-coated structures with low current demand,** or to protect a local hot spot [1].
- **Congested areas,** where an impressed current groundbed could interfere with other buried metal [1][2].
- **Large offshore structures,** where NPL notes galvanic protection of uncoated platforms has proved cost effective and works from the moment the structure is floated out, without a power supply [1].
- **Particular materials and settings.** Magnesium suits buried use and aluminum and zinc mainly marine use [1]; zinc anodes are used on prestressed concrete pipe because impressed current could embrittle the prestressing steel [2].

## When is impressed current used?

- **Long pipelines and large, complex structures,** including bare or poorly coated ones [1].
- **High-resistivity soils,** where the small galvanic driving voltage cannot push enough current [1][3].
- **Changing demand,** because rectifier output can be raised as coatings age or the structure grows [1]. In variable waters such as tidal estuaries, output can be controlled automatically from a permanent reference electrode [1].

## How is either system checked?

The same criteria apply to both. For steel under Part 192, Appendix D accepts, among other criteria, a potential at least 0.85 V more negative than a saturated copper-copper sulfate reference cell with current applied, allowing for voltage drops, or at least 100 mV of polarization measured by interrupting the current [6]. Hazardous liquid lines use the criteria in NACE SP0169 that 49 CFR 195.571 references [7]. NPL adds that steel exposed to sulfate-reducing bacteria needs a more negative potential, about -0.95 V against copper-copper sulfate [1].

Close interval surveys measure pipe-to-soil potential every few feet, either switching the current on and off, after depolarization, or with current on where it cannot be interrupted [8][9]. When an annual test station reading on an onshore gas transmission line is low and the cause is systemic, the operator must run such a survey in both directions, at about 5-foot spacing, normally with the current interrupted (49 CFR 192.465) [5]. NPL considers a twice-yearly check, including sacrificial anodes, generally sufficient, and notes that about 5% of test posts are damaged each year [2].

## Where integrity problems show up

| Where it occurs (unit or equipment) | Conditions that drive it | How it is usually found | In the Library |
|---|---|---|---|
| Coated gas line in rock backfill under impressed current [8] | Rocks damaged the coating and shielded the steel; test station 100 feet away read satisfactory [8] | In-line inspection or pressure testing, which the NTSB concluded would likely have revealed it [8] | [Pipe-to-soil potential](/glossary/pipe-to-soil-potential/) |
| Foreign pipelines, cables or moored vessels near a protected structure | Protective current picked up and discharged by the other structure corrodes it where it leaves [1] | Interference tests, usually yearly where at risk or after output changes [1]; interference surveys on gas transmission lines (49 CFR 192.473) [5] | What is soil corrosion? |
| Rectifier-powered systems | Protection lasts only while amperage and voltage are maintained [5] | Rectifier inspections six times a year, remotely or on site, plus a yearly physical check of remote units (49 CFR 192.465) [5] | [Impressed current cathodic protection](/glossary/impressed-current-cathodic-protection/) |
| Galvanic systems as coatings deteriorate | Current demand rises but anode output cannot be raised [1] | Annual potential tests and anode current measured at test posts [1][5] | [Sacrificial anode](/glossary/sacrificial-anode/) |
| High-strength steels, some corrosion-resistant alloys, prestressed concrete pipe | Excessive negative potential releases hydrogen that can embrittle the steel [1][2] | Potential measurements compared with the limits set for the structure [1] | [What is hydrogen embrittlement?](/library/hydrogen-embrittlement/) |

Sources: NTSB PAR-14/01 [8]; NPL Guides No. 1 and 4 [1][2]; 49 CFR 192 Subpart I [5].

## Sources

1. [Guides to Good Practice in Corrosion Control No. 1: Cathodic Protection (D. W. Harvey), National Physical Laboratory (NPL), UK](https://eprintspublications.npl.co.uk/8402/1/Corrosion%20Guide%20No%201.pdf)
2. [Guides to Good Practice in Corrosion Control No. 4: Corrosion Control for Buried Pipelines (D. W. Harvey), National Physical Laboratory (NPL), UK](https://eprintspublications.npl.co.uk/8622/1/Corrosion%20Guide%20No%204.pdf)
3. [TM 5-811-7, Electrical Design, Cathodic Protection (Technical Manual), Headquarters, US Department of the Army (hosted by the Whole Building Design Guide)](https://www.wbdg.org/FFC/ARMYCOE/COETM/tm_5_811_7.pdf), 1985-04-22
4. [Fact Sheet: Cathodic Protection, US Pipeline and Hazardous Materials Safety Administration (PHMSA)](https://primis.phmsa.dot.gov/stakeholder-comms/factsheets/fscathodicprotection)
5. [49 CFR Part 192, Subpart I, Requirements for Corrosion Control (192.455 to 192.473), eCFR, US Office of the Federal Register](https://www.ecfr.gov/current/title-49/chapter-I/subchapter-D/part-192/subpart-I)
6. [Appendix D to Part 192, Criteria for Cathodic Protection and Determination of Measurements, eCFR, US Office of the Federal Register](https://www.ecfr.gov/current/title-49/chapter-I/subchapter-D/part-192/appendix-Appendix%20D%20to%20Part%20192)
7. [49 CFR Part 195, Subpart H, Corrosion Control (195.563 to 195.577), eCFR, US Office of the Federal Register](https://www.ecfr.gov/current/title-49/chapter-I/subchapter-D/part-195/subpart-H)
8. [Pipeline Accident Report NTSB/PAR-14/01: Columbia Gas Transmission Corporation Pipeline Rupture, Sissonville, West Virginia, December 11, 2012, US National Transportation Safety Board (NTSB)](https://www.ntsb.gov/investigations/AccidentReports/Reports/PAR1401.pdf)
9. [Fact Sheet: Close Interval Survey, US Pipeline and Hazardous Materials Safety Administration (PHMSA)](https://primis.phmsa.dot.gov/stakeholder-comms/factsheets/fscloseinternalsurvey)

Published by Winda Beacon (https://beacon.winda.ai).