# What is short-term overheating of heater tubes?

> Short-term overheating is rapid failure of a heater or boiler tube running far above its design temperature, usually after loss of flow or overfiring. The hot wall loses strength, bulges under internal pressure and ruptures within minutes to days. API RP 571 describes it among refinery damage mechanisms, and API Std 530 covers heater tube thickness.

- Label: Fact
- Type: Explainer
- Published: 2026-11-13T09:44:04+09:00
- By: Jun Zhong
- Researched and drafted by: Beacon's AI newsroom
- Checked by: Jun Zhong on 2026-11-13
- Topics: Refining
- Canonical: https://beacon.winda.ai/library/short-term-overheating/

## Why does it matter?

Shortly after midnight on 19 November 2023, a tube ruptured in the fired heater of a renewable diesel hydroprocessing unit in Martinez, California, during the unit's first start-up in that service [1]. The stainless steel tubes had been installed new less than two weeks earlier; thermocouples read up to 1,710 °F (932 °C) against a design temperature of 1,120 °F (604 °C), and metallurgical analysis put the failed tube at about 1,500 to 2,000 °F (816 to 1,093 °C) [1]. Renewable diesel and hydrogen escaped and burned, a field operator was seriously injured, and property damage was about $350 million [1][2]. The US Chemical Safety and Hazard Investigation Board (CSB) counted seven other fired heater tube ruptures reported to it from 2020 through 2024, at least five from the same mechanism [1].

## What happens to an overheated tube?

A heater tube's wall is made thick enough to contain the process pressure up to a set design temperature; the Martinez tubes were designed with API Std 530 [1][6]. Well above that temperature the steel loses much of its strength, and the internal pressure pushes the wall outward: the diameter grows, the wall thins, the metal weakens further, and a local bulge forms [1]. The bulge then splits open in what is called a "fish-mouth" rupture [1]. Post-incident metallurgical analysis at Martinez identified the mechanism as short-term overheating, a stress rupture that is sometimes called hot tensile rupture [1].

Basson and Fuls (2021) note that, depending on how hot the tube gets, failure can come within minutes or over a few days, and that the burst tube typically shows a thin-lipped fish-mouth opening and discoloration from local heating [3]. Those features set it apart from long-term overheating, or creep [3].

## What causes it?

| Cause | What happens | Example or source |
|---|---|---|
| Loss of flow through the tubes | The process fluid no longer carries heat away from the tube wall | At Martinez, an open valve sent much of the flow around the heater, downstream of the flow meter that fed the low-flow trip [1] |
| Afterburning or poor combustion | Unburned fuel burns higher in the heater and overheats tubes there | Two of the four lit burners had their air inlets covered by plates, and the convection tubes overheated [1][2] |
| Fouling and coke inside tubes | Deposits restrict flow and heat transfer | Inadequate crude desalting fouls heater tubes and leads to failures from higher pressures and temperatures [4] |
| Low water or blocked steam in boilers | Tubes lose their cooling | Boiler tubes overheat and fail if feedwater runs low; superheaters need care at start-up and shutdown [4]; flaking oxide scale can block superheater bends [5][3] |

## How is it detected before a rupture?

- **Tube metal temperature.** Thermocouples attached to the outer surface of the tubes measure metal temperature; the Martinez heater had ten, with six in the radiant section and four higher up in the convection section [1]. The CSB found tube metal temperature a more direct sign of overheating than process outlet temperature, and noted industry guidance against relying on outlet temperature to detect lost flow [1].
- **Infrared scans.** An infrared camera can estimate tube temperatures but needs suitable equipment, training and a "trained eye" [1]. At Martinez a supervisor scanned the outside of the heater instead of the tubes, and his lower readings led the board operator to believe the displayed tube temperatures could be about 300 °F (about 167 °C) too high [1].
- **Flow and combustion.** The low-flow trip at Martinez could not see the bypass, because its flow meter sat upstream of the point where flow left the heater path [1]. The heater had a combustibles analyzer at the bridgewall, but its readings showed only on a local panel and were not recorded [1].
- **After an event.** Diameter measurements found bulging around the rupture and in nearby tubes that had not failed [1].

## What did investigators recommend?

These are the CSB's recommendations, not Beacon's. The CSB called for alarms on tube metal temperature tied to predefined actions, including remote shutdown and moving people away from the heater; safeguards against afterburning that can be watched from the control room; design requirements that protect heaters from low flow where piping branches downstream of a flow meter; "walk the line" checks of valve positions before start-ups; and a revision of API RP 556, the recommended practice on how gas-fired heaters are instrumented, controlled and protected, to address high tube temperatures, flow diversion and afterburning [1][2].

## Where integrity problems show up

| Where it occurs (unit or equipment) | Conditions that drive it | How it is usually found | In the Library |
|---|---|---|---|
| Fired heater radiant and convection tubes | Lost flow or afterburning drives metal far above design [1] | Tube metal thermocouples; infrared scans by trained staff [1] | What is a fired heater? |
| Charge heaters of hydroprocessing units at start-up | Start-up piping can divert flow around the heater unseen [1] | Flow measured where a bypass would show; tube metal temperature [1] | [What is hydroprocessing (hydrotreating and hydrocracking)?](/library/hydroprocessing/) |
| Crude unit heater tubes | Fouling after poor desalting [4] | Tube metal temperature monitoring [1] | [What is a crude distillation unit?](/library/crude-distillation-unit/) |
| Boiler superheater tubes | Oxide flakes blocking bends; condensate at start-up [5][3] | Appearance of the burst tube; blockage modeling [3][5] | [What is high-temperature oxidation?](/library/high-temperature-oxidation/) |
| Tubes next to a rupture | Same overheating, short of failure [1] | Outer diameter measurement of every tube [1] | What are the main non-destructive testing (NDT) methods in oil and gas? |
| Heaters with no limit set for tube temperature | No not-to-exceed limit for tube metal temperature at Martinez [1] | Alarms with predefined responses, as the CSB recommended [1] | [What are integrity operating windows (IOWs)?](/library/integrity-operating-windows/) |

Sources: CSB, 2025 [1][2]; Basson and Fuls, 2021 [3]; OSHA Technical Manual [4]; ORNL, 2014 [5].

## Sources

1. [Investigation Report: Fired Heater Tube Rupture and Fire at Marathon Martinez Renewables Facility, Martinez, CA (No. 2024-01-I-CA), US Chemical Safety and Hazard Investigation Board (CSB)](https://www.csb.gov/assets/1/6/Marathon_Martinez_2025-03-12_ForPublication.pdf)
2. [CSB Issues Final Report Into 2023 Fire at the Marathon Renewables Facility in Martinez, California (news release), US Chemical Safety and Hazard Investigation Board (CSB)](https://www.csb.gov/us-chemical-safety-board-issues-final-report-/), 2025-03-13
3. [Over-attemperation and Short-term Overheating in Pendant-type Superheaters (N. Basson, W. F. Fuls), R&D Journal of the South African Institution of Mechanical Engineering 37, 58-69, South African Institution of Mechanical Engineering (open access, CC BY 4.0)](https://rdj.journals.ac.za/index.php/pub/article/view/21)
4. [OSHA Technical Manual, Section IV, Chapter 2: Petroleum Refining Processes, US Occupational Safety and Health Administration (OSHA)](https://www.osha.gov/otm/section-4-safety-hazards/chapter-2)
5. [Managing Oxide Scale Exfoliation in Boilers with TP347H Superheater Tubes (A. S. Sabau, I. G. Wright, J. P. Shingledecker, P. F. Tortorelli), conference paper (record and abstract), Oak Ridge National Laboratory, via US DOE Office of Scientific and Technical Information (OSTI)](https://www.osti.gov/biblio/1126527)
6. [2025 Publications Catalog (entries for RP 571, Std 530 and RP 573) (RP 571, 3rd edition, March 2020; Std 530, 7th edition, April 2015 (with addenda of July 2019 and December 2021); RP 573, 4th edition, 2021), American Petroleum Institute (API)](https://www.api.org/-/media/files/publications/2025-catalog/2025_pubs%20catalog.pdf)

Published by Winda Beacon (https://beacon.winda.ai).