What is cavitation damage?

·3 sources

Short answer

Cavitation damage is metal loss caused when vapor bubbles, formed where a liquid's pressure falls below its vapor pressure, collapse against a surface. The collapse fires tiny high-speed jets and pressure waves at the metal. It attacks pump impellers and casings, valves with large pressure drops and the pipe just downstream.

By , Editor·Researched and drafted by ·Checked by , Editor·Last checked ·Next review

Why does it matter?

A centrifugal pump running at exactly its rated net positive suction head required (NPSHR) is already cavitating: in the Hydraulic Institute definition cited by the US Department of Energy (DOE), NPSHR is the suction head at which cavitation has already cut the pump's head by 3% 1. Sustained cavitation erodes the impeller, which can go out of balance and speed bearing wear, and the vibration it causes loads foundations and connected piping 1. Because it shortens pump life so sharply, the DOE ranks cavitation as a serious threat to system reliability 1.

What causes cavitation?

When a liquid speeds up, its static pressure drops. If the pressure falls to the liquid's vapor pressure, the liquid boils locally into small vapor bubbles; when the flow carries them into higher pressure, they turn back to liquid by collapsing violently 1. Researchers at the US National Aeronautics and Space Administration (NASA) describe the damage as impacts from microjets or shock waves, depending on how far the collapse is from the surface 3.

The impact force often exceeds the strength of the metal, so material is torn out 1. Cavitation can occur in any liquid, including oils 3.

In pumps, the DOE names these conditions 1:

  • High flow, with the pump running far to the right on its performance curve. 1
  • Hotter fluid than the design temperature, or lower suction pressure than the design value. 1
  • Starved suction, from air pockets or fouled suction pipes. 1
  • Low flow, where vortices and internal recirculation cause cavitation-like damage on the impeller vanes. 1

In valves, cavitation follows control valves that take a large pressure drop 2. Throttling the excess flow of an oversized pump wears valve seats through throttling and cavitation 1.

The NPSH margin. A pump needs a minimum pressure at its inlet to avoid cavitation, called net positive suction head (NPSH) 1. The system supplies NPSH available (NPSHA); the pump needs NPSHR 1. Near the pump's best efficiency point a small margin is usually enough, but away from it a much larger margin is needed to suppress all cavitation; a common design rule cited by the DOE is NPSHA at least 25% above NPSHR across expected flows 1.

What does cavitation damage look like?

The metal is pitted and roughened rather than evenly thinned. In NASA laboratory tests, pits formed first at grain boundaries and around precipitates, pits where three grains meet grew fastest, and craters roughened the grain surfaces 3. Each metal showed an incubation period before erosion took off, very short for some and longest for a titanium alloy 3. Local metal loss in service can be severe 2.

Materials differ widely. In the NASA tests, aluminum alloy, copper, brass, bronze and nickel eroded 10 to 100 times faster than a titanium alloy, while iron and molybdenum fell in between 3. The DOE notes that tougher, higher-tensile-strength impeller materials withstand more energetic cavitation 1.

How is cavitation found?

  • Noise. Crackling and popping, often compared to marbles passing through the pump, signal cavitation 1.
  • Performance. Vapor restricts flow and lowers the head the pump generates 1.
  • Vibration and wear. Vibration analysis is one of the preventive maintenance techniques the DOE lists for bearings, and cavitation shows up as unbalance and faster bearing and seal wear 1.
  • Valve condition. Seat wear from throttling and cavitation shortens the interval between valve overhauls 1.

How is cavitation prevented?

  • Suction conditions. Keep NPSHA above NPSHR with margin over the full flow range; near the best efficiency point a small margin suffices, while oversized pumps running far right on their curves can shrink the margin to a dangerous level 1.
  • Design of pumps and valves. Lay out pressure and flow inside the components so that cavitation does not occur, and keep gaskets from protruding into the flow 2. The UK National Physical Laboratory notes that careful design usually avoids cavitation except under abnormal operating conditions 2.
  • Materials. Where some cavitation cannot be avoided, the DOE recommends tougher impeller materials that are also compatible with the fluid 1.

Where integrity problems show up

Where it occurs (unit or equipment)Conditions that drive itHow it is usually foundIn the Library
Centrifugal pump impellers and casingsInlet pressure below vapor pressure: high flow, hot fluid, low suction pressure, starved suction 1Crackling noise, lost head, vibration 1What is predictive maintenance in oil and gas?
Pumps run at low flowVortices and internal recirculation on impeller vanes 1Vibration analysis, bearing and seal wear 1What is mechanical and vibration fatigue?
Control and throttling valves with large pressure dropsPressure falls through the valve and recovers downstream 1,2Valve seat wear and shorter overhaul intervals 1Preventive vs predictive vs corrective maintenance
Piping just downstream of valves and pumpsBubbles collapsing as pressure recovers; erosion of pipe surfaces 1,2Noise in pipes and across valves, pipe vibration 1How does ultrasonic thickness measurement work?

Sources: DOE pump sourcebook, 2006 1; NPL Guide No. 6 2; NASA TP-2368, 1984 3.

Common questions

Is cavitation the same as erosion-corrosion?
No. Erosion-corrosion, or impingement attack, happens when turbulent flow or entrained solids strip the protective film and the metal then corrodes, leaving smooth, water-swept pits. Cavitation is mechanical damage from collapsing vapor cavities. See [Corrosion vs erosion vs erosion-corrosion: what is the difference?](/library/corrosion-vs-erosion/).
Does a corrosion-resistant alloy stop cavitation?
Not by itself. Resistance depends on strength and microstructure; in NASA tests a titanium alloy eroded far more slowly than nickel or copper alloys, and the DOE points to tougher, higher-strength materials.
What is NPSH?
Net positive suction head is the inlet pressure margin that keeps liquid from boiling in the pump. The system provides NPSH available; the pump needs NPSH required, read from its performance curve.

Beacon explains these concepts in its own words for education. It does not reproduce or replace the standards cited, and Winda is not affiliated with or endorsed by the organizations that publish them. Engineering decisions need the current edition of the standard and a qualified engineer.

Sources

  1. 1.Improving Pumping System Performance: A Sourcebook for Industry, Second Edition (DOE/GO-102006-2079) · US Department of Energy, Industrial Technologies Program, and the Hydraulic Institute (prepared by Lawrence Berkeley National Laboratory)
  2. 2.Guides to Good Practice in Corrosion Control No. 6: Corrosion Control for Pumps and Valves · UK National Physical Laboratory (NPL)