What is pulsed eddy current (PEC) testing?
Pulsed eddy current (PEC) testing measures the average wall thickness of carbon and low-alloy steel through insulation, without touching the metal. A coil sends a magnetic pulse, and the way the induced eddy currents die away is compared with calibration readings. It is used mainly to screen for corrosion under insulation (CUI).
By Jun Zhong, Editor·Researched and drafted by Beacon's AI newsroom·Checked by Jun Zhong, Editor·Last checked ·Next review
Why does it matter?
A PEC reading is an average. UK Health and Safety Executive (HSE) guidance describes the result as the average wall loss over the probe's footprint, unlike a point reading from ultrasonic thickness measurement 1. The method is chosen to avoid stripping insulation: while investigating a 2018 generator fire on an offshore platform, whose cause was inconclusive, the US Bureau of Safety and Environmental Enforcement (BSEE) found severe corrosion under insulation on exhaust piping and noted that inspecting insulated components may require removing guards and insulation 5. PEC can show whether general wall loss is present; it does not show how deep the worst pit is 2.
How does PEC work?
PEC drives the coil with a step or short pulse instead. A step contains a continuous range of frequencies, so one pulse samples a range of depths, and features farther from the coil show up later in time 3.
The pulse induces eddy currents in the steel; as they spread through the wall and decay, they produce a second magnetic field that a receiving coil picks up 1. How fast the signal decays depends on the material and the wall thickness. Comparing the decay with readings on calibration pieces removes the material effect and leaves an average thickness for the area under the probe 1,2.
A 2003 study for the US Minerals Management Service (MMS) reported that one reading takes a couple of seconds, that probes of about 50 to 100 mm diameter were used, and that logged readings can be repeated later at the same spots 2.
Where is PEC used?
- Offshore risers. The MMS study described PEC finding wall-thinning areas on risers through protective coatings and marine growth, without cleaning, and noted that systems can work under water 2.
- The middle step of a screening sequence. The MMS study described long-range ultrasonic screening first, then local PEC or digital radiography for a closer estimate, then automated ultrasonic mapping for the most accurate measurement 2.
What are its limits?
- Material. HSE describes PEC as suitable only for low-alloy steels 1.
- No surface discrimination. PEC cannot tell whether wall loss is on the near or far side 1.
- Geometry. The MMS study cited walls of 6 to 65 mm and insulation under 150 mm 2.
- Jacketing. Simulations in the 2022 review found stronger signals under aluminum jacketing than under stainless steel 4.
- Status as a screening tool. In 2003 the MMS study placed PEC and long-range ultrasonics below a "fairly effective" rating for measuring corrosion rate, because of measurement uncertainty and unknown probability of detection, and said screening should find significant wall loss, not set rates 2.
- Set-up. HSE notes that operators need information about the component to set up the equipment and interpret results 1.
Where integrity problems show up
| What it finds well | What it can miss or get wrong | In the Library |
|---|---|---|
| General wall loss under insulation, with the insulation left on 1 | Small, isolated pits inside the probe footprint 4 | What is corrosion under insulation (CUI)? |
| Riser wall loss through coatings and marine growth, also under water 2 | A reliable corrosion rate: the 2003 study ranked screening tools below fairly effective for rates 2 | Corrosion rate |
| Wall loss in carbon and low-alloy steel 1 | Other alloys, for which HSE lists it as unsuitable 1 | Carbon steel vs stainless steel in process service |
| The presence of thinning 1 | Whether thinning is internal or external, which needs a follow-up method 1 | How does ultrasonic thickness measurement work? |
Sources: HSE COMAH technical measures document 1; MMS riser study, 2003 2; Cao et al., 2022 4.
Common questions
- Is PEC the same as eddy current testing?
- It is a form of it. Conventional eddy current testing uses one frequency and, in steel, sees only the surface layer, while PEC uses a pulse that carries many frequencies and reaches through the wall.
- Does the insulation or jacketing have to come off?
- Not for the PEC reading itself, as long as the layers are non-conductive and non-magnetic; HSE gives up to 100 mm of such material, such as passive fire protection or concrete. Confirming a finding with a contact method usually needs access to the metal.
- How is PEC different from guided wave testing for CUI?
- Guided waves travel along a pipe from one probe position and screen long lengths for signs of wall loss, while PEC gives spot readings of average thickness. See [Guided wave testing](/glossary/guided-wave-testing/).
Beacon explains these concepts in its own words for education. It does not reproduce or replace the standards cited, and Winda is not affiliated with or endorsed by the organizations that publish them. Engineering decisions need the current edition of the standard and a qualified engineer.
Sources
- 1.Inspection/Non Destructive Testing (COMAH technical measures document) · UK Health and Safety Executive (HSE)
- 2.Evaluation of Methods for Detecting and Monitoring of Corrosion and Fatigue Damage in Risers (M. Lozev, B. Grimmett, E. Shell, R. Spencer), Technical Assessment Program project 433 · US Minerals Management Service (now Bureau of Safety and Environmental Enforcement, BSEE) ·
- 3.Pulsed Eddy Current Inspection (NDE-Ed) · Iowa State University, Center for Nondestructive Evaluation
- 4.A Review of Corrosion under Insulation: A Critical Issue in the Oil and Gas Industry (Q. Cao et al.), Metals 12(4):561 · MDPI (open access, CC BY 4.0)