What is under-deposit corrosion?
Under-deposit corrosion (UDC) is localized corrosion of steel beneath sand, scale, sludge, iron sulfide or biofilm settled inside a pipe or vessel. The deposit changes the chemistry at the wall and can block corrosion inhibitors, so pits can grow under it much faster than on the open wall.
By Jun Zhong, Editor·Researched and drafted by Beacon's AI newsroom·Checked by Jun Zhong, Editor·Last checked ·Next review
Why does it matter?
In February 2012, sour gas piping on an offshore platform in the Santa Maria Basin off California failed next to a weld and released gas carrying an estimated 40,000 parts per million (ppm) of hydrogen sulfide (H2S) 1. Ten years of ultrasonic readings on that piping circuit had shown no appreciable wall loss 1. Investigators for the US Bureau of Safety and Environmental Enforcement (BSEE) traced the failure to fast, local corrosion in a low-flow reducer where deposits could build up 1. The readings had been taken on smooth pipe away from the weld, and BSEE noted that the heavy scale may also have affected their accuracy 2.
How do deposits cause corrosion?
Produced fluids carry sand, silt and other solids, and these settle along the bottom of a line wherever the flow is too slow to keep them moving 3. A deposit then works against the steel in several ways:
- It isolates the wall. The deposit slows the exchange of species between the liquid and the steel, so the water at the wall no longer matches the bulk fluid 3.
- It blocks treatment chemicals. Inhibitors and biocides reach the bare wall but struggle to get through the deposit, and the deposit's own large surface soaks some of them up 3.
- It sets up a galvanic cell. Once the open wall is inhibited, it becomes the cathode and the small area under the deposit the anode. A review of laboratory work found that a sand bed only 1% of the pipe diameter deep in an inhibited water injection line leaves almost 15 times more cathode area than anode area 3.
- It starves oxygen. In aerated water, the area under a deposit gets less oxygen and corrodes as the anode of an oxygen cell 8.
- It shelters microbes. Deposits give bacteria a habitat; in a 2022 laboratory study, areas under bacterial iron deposits on carbon steel were anodic and pitted, even with an inhibitor present 4.
What kinds of deposits are involved?
| Deposit type | Examples | What it does | Source |
|---|---|---|---|
| Inert solids | Sand, silt, clay, some scales | Act as a diffusion barrier and keep inhibitor off the wall | 3 |
| Conductive solids | Iron sulfides such as mackinawite, pyrrhotite and pyrite | Conduct electrons and can drive galvanic attack; a field sludge containing mackinawite gave average rates of 30 mm per year (mm/y) beneath it in a 24-hour laboratory test, against under 1 mm/y without deposit | 3 |
| Organic and mixed | Wax, asphaltenes, and "schmoo" (solids bound with oil) | Form a physical barrier; schmoo is a habitat for bacteria | 3 |
| Biological | Biofilms and iron deposits made by bacteria | Local anodes, pitting and breakdown of inhibitor films | 4 |
| Elemental sulfur in scale | Sulfur formed when oxygen enters wet sour gas | Acts as an oxidizer and causes local attack | 1,2 |
How is under-deposit corrosion found?
- Thickness readings need to cover the right spots. In the 2012 case, ultrasonic readings at fixed points missed the attack near the weld, and BSEE recommended radiography where ultrasonic testing is difficult, such as at welds, reducers and flanges 1,2.
- Pig returns and samples. The US National Transportation Safety Board (NTSB) notes that sampling the liquids and solids removed from a pipeline can reveal corrosive contaminants, including bacteria, and that internal corrosion can be found by visual examination of opened pipe, wall thickness measurement, coupons or probes, and in-line inspection 5.
- Removed pipe. US gas pipeline rules require the inside of any pipe removed from a line to be inspected for corrosion (49 CFR 192.475(b)) 7.
How is under-deposit corrosion controlled?
- Design. A 2017 review lists designing for higher flow, avoiding stagnant spots, adding pigging facilities, and using corrosion-resistant alloys or internal coatings 3.
- Cleaning. Pigging, often with brush pigs and a batch of inhibitor, removes deposits; the same review warns that a large sand load pushed ahead of a pig can plug a line 3. PHMSA lists cleaning pigs among routine measures against internal corrosion 6.
- Chemistry. Inhibitors are chosen by laboratory testing and field trials 3.
- Keep oxygen out of sour systems. After the 2012 release, the operator was advised to eliminate oxygen entry at compressor and pump seals, wash water and glycol 1.
Where integrity problems show up
| Where it occurs (unit or equipment) | Conditions that drive it | How it is usually found | In the Library |
|---|---|---|---|
| Offshore sour gas piping at reducers, flanges and welds | Low flow, heavy scale, elemental sulfur from oxygen ingress 1 | Radiography where ultrasonic readings at fixed points are unreliable 1,2 | Radiographic testing |
| Low points in gas transmission pipelines | Liquids and solids collecting where pipe bending made a sag; chloride-rich deposits and bacteria 5 5 | Sampling pig returns, wall thickness measurement, coupons or probes, in-line inspection 5 | What is in-line inspection (ILI) and pigging? |
| Production and water injection lines carrying sand | A sand bed under an inhibited flow 3 | In-line inspection; cleaning pig returns show what settles 3,6 | How do corrosion inhibitors work? |
| Gas pipelines carrying corrosive gas | Water and contaminants in the gas 7 | Coupons or other monitoring checked twice each calendar year (49 CFR 192.477) 7 | Corrosion coupons vs electrical resistance (ER) probes |
Sources: BSEE OCS Report 2012-104 1; NTSB PAR-03/01, 2003 5; Brown and Moloney, 2017 3; 49 CFR 192.475 and 192.477 7.
Common questions
- Is under-deposit corrosion the same as microbiologically influenced corrosion (MIC)?
- No. Deposits can drive corrosion with no microbes at all, for example through an inhibitor-driven galvanic cell or elemental sulfur. But deposits are good habitats for bacteria, so the two often occur together. See [What is microbiologically influenced corrosion (MIC)?](/library/microbiologically-influenced-corrosion/).
- Can a corrosion inhibitor make under-deposit corrosion worse?
- It can. Laboratory work shows that an inhibitor lowers corrosion on the open wall but may not reach steel under a deposit, which then becomes a small anode coupled to a large protected cathode.
- How is it different from crevice corrosion?
- Both happen in shielded spots, and a deposit can act as a crevice. Under-deposit corrosion in pipelines also involves inhibitor shielding, conductive iron sulfides and microbes.
Beacon explains these concepts in its own words for education. It does not reproduce or replace the standards cited, and Winda is not affiliated with or endorsed by the organizations that publish them. Engineering decisions need the current edition of the standard and a qualified engineer.
Sources
- 1.OCS Report BSEE 2012-104, Investigation of H2S Gas Release, Platform Hidalgo, OCS-P 0450, Pacific OCS Region · US Bureau of Safety and Environmental Enforcement (BSEE)
- 2.Safety Alert No. 22, Hydrogen Sulfide (H2S) Gas Release from Piping Corrosion Failure Near a Weld · US Bureau of Safety and Environmental Enforcement (BSEE) ·
- 3.Under-deposit corrosion (B. Brown, J. Moloney), chapter 15 in Trends in Oil and Gas Corrosion Research and Technologies · Elsevier (Woodhead), hosted by Ohio University Institute for Corrosion and Multiphase Technology
- 4.In Situ Investigation of Under-Deposit Microbial Corrosion and its Inhibition Using a Multi-Electrode Array System (E. M. Suarez and others), Frontiers in Bioengineering and Biotechnology 9, 803610 · Frontiers (open access, CC BY), via PubMed Central ·
- 5.Pipeline Accident Report NTSB/PAR-03/01, Natural Gas Pipeline Rupture and Fire Near Carlsbad, New Mexico, August 19, 2000 · US National Transportation Safety Board (NTSB) ·
- 6.Fact Sheet: Internal Corrosion · US Pipeline and Hazardous Materials Safety Administration (PHMSA)
- 7.49 CFR 192.475, Internal corrosion control: General, and 49 CFR 192.477, Internal corrosion control: Monitoring · eCFR, US Office of the Federal Register
- 8.Forms of Corrosion · NASA Kennedy Space Center, Corrosion Technology Laboratory