Skip to content
Beaconby Winda
FactCorrosion and Damage Mechanisms · Environmental cracking

What is wet hydrogen sulfide (H2S) damage?

·8 sources

Short answer

Wet hydrogen sulfide (H2S) damage is hydrogen damage to carbon steel in water that contains H2S. Corrosion releases hydrogen into the steel, causing blistering, sulfide stress cracking (SSC), hydrogen-induced cracking (HIC) and its stress-oriented form (SOHIC). NACE MR0175/ISO 15156 sets material requirements for H2S service in oil and gas production.

By , Editor·Researched and drafted by ·Checked by , Editor·Last checked ·Next review

Why does it matter?

On July 23, 1984, an amine absorber at a refinery in Romeoville, Illinois, ruptured; 17 people died, and OSHA reported damage of more than $100 million 4. Investigators at the National Bureau of Standards (now NIST) found that cracks had started in hard metal formed during a repair weld, then grown through more than 90% of the wall by hydrogen pressure cracking 3. Hydrogen had also cut the steel's fracture resistance by more than half, so the vessel broke at about 10% of the steel's rated strength, although measured wall thicknesses were within allowances 3.

How does wet H2S damage steel?

When steel corrodes in water containing H2S, hydrogen is produced at the surface and part of it enters the metal as atoms 1. Inside, the atoms collect at traps such as inclusions, voids and grain boundaries, recombine into hydrogen gas and build internal pressure 7. Dissolved hydrogen can also lower ductility and fracture toughness without any visible flaw 2. Sensitivity rises with the hardness and strength of the steel 1,2.

What forms does wet H2S damage take?

FormWhat it looks likeWhat drives it
Hydrogen blisteringSurface bulges over internal voids parallel to the surface; a sign that hydrogen is entering 2Hydrogen gas collecting near the surface 2

Sources: NIST SP 780, 1990 2; Kazys and others, 2022 7.

Where does wet H2S damage occur?

  • Refinery pressure vessels. A 1988 interim report from a refinery industry inspection program found cracks of varying severity in 31% of 189 vessels, more than expected, partly because a more sensitive examination method was used 2.
  • Liquefied petroleum gas (LPG) storage spheres. A survey reported cracking in 30% of 141 vessels, part of it old fabrication flaws but part in-service cracking, mostly in weld heat-affected zones. The H2S was carried over from upstream treating, and incidence was higher in as-welded and higher-strength steels 2.
  • Crude, catalytic cracking and gas plants. OSHA notes that wet H2S cracks steel in crude unit service, and that ammonia and cyanide from high-nitrogen feeds can cause corrosion, cracking or hydrogen blistering in catalytic cracking overhead systems 8.

How is wet H2S damage found?

  • Wet fluorescent magnetic particle testing (WFMT) of internal weld surfaces was the method used in the refinery inspection program and is more sensitive than older methods 2.
  • Visual examination shows blistering on a clean, well-lit surface 1.
  • Ultrasonic testing finds internal cracks. In a 1990s research program on welded plates in wet H2S, several ultrasonic methods used together sized HIC, SOHIC and SSC well, automated scans were more repeatable than manual ones, and no single method described the damage fully 5,6.
  • Newer ultrasonic imaging. A 2022 study on refinery exchanger steel found total focusing method imaging resolved cracks close to 0.2 mm, and a low-angle time-of-flight diffraction probe suited screening large areas 7.
  • Hardness testing has a known gap: significant cracks can start from very small hard zones at welds that conventional hardness tests do not detect 1.

What limits it?

Measures described in US government guidance and industry sources include lower-strength steels for new vessels, weld hardness control, post-weld heat treatment (PWHT), which appears to reduce sensitivity to cracking and its severity, and better monitoring of H2S carry-over 1,2. OSHA notes that weld hardness limits may not fully prevent cracking 1.

Where integrity problems show up

Where it occurs (unit or equipment)Conditions that drive itHow it is usually foundIn the Library
Refinery vessels in wet H2S serviceWater with H2S; hard zones at welds; no PWHT 1,2Internal WFMT of welds; ultrasonic testing for internal cracks 1,2,6Hydrogen induced cracking
LPG storage spheresH2S carry-over; as-welded, higher-strength steel 2WFMT; early inspection of spheres more than 5 years in service 1,2Sulfide stress cracking
Amine absorbers and vessels repaired without PWHTHard repair-weld zones; hydrogen 3,4Magnetic particle testing showed hundreds of weld cracks; ultrasonic testing showed internal separation 3What is amine corrosion and amine cracking?
Catalytic cracking overhead systemsMoist H2S with ammonia and cyanide from high-nitrogen feed 8Visual examination for blistering 1What is fluid catalytic cracking (FCC)?

Sources: OSHA Technical Manual, Section IV, Chapters 2 and 3 1,8; NIST SP 780, 1990 2; NIST SP 958 3; OSTI 403561 6.

Common questions

What is the difference between HIC, SOHIC and SSC?
HIC is stepwise cracking in the rolling plane that needs no stress; SOHIC is HIC lined up and linked through the wall by stress; SSC is cracking of hard steel under tensile stress, controlled mainly through hardness limits. See [HIC vs SOHIC vs SSC](/library/hic-vs-sohic-vs-ssc/).
Is wet H2S damage the same as high temperature hydrogen attack?
No. Wet H2S damage comes from hydrogen produced by corrosion in water. High temperature hydrogen attack is a reaction between hot hydrogen gas and carbon in steel; see [What is high temperature hydrogen attack (HTHA)?](/library/high-temperature-hydrogen-attack/).
Does post-weld heat treatment prevent wet H2S cracking?
It reduces the risk but does not remove it. NIST and OSHA summarize survey findings that PWHT appears to reduce sensitivity to cracking and its severity.

Beacon explains these concepts in its own words for education. It does not reproduce or replace the standards cited, and Winda is not affiliated with or endorsed by the organizations that publish them. Engineering decisions need the current edition of the standard and a qualified engineer.

Sources

  1. 1.OSHA Technical Manual, Section IV, Chapter 3: Pressure Vessel Guidelines · US Occupational Safety and Health Administration (OSHA)
  2. 2.NIST Special Publication 780, Guidelines for Pressure Vessel Safety Assessment (S. Yukawa) · US National Institute of Standards and Technology (NIST)
  3. 3.Analysis of the Catastrophic Rupture of a Pressure Vessel (prepared by T. Siewert), in NIST SP 958, A Century of Excellence in Measurements, Standards, and Technology, pp. 350-352 · US National Institute of Standards and Technology (NIST)
  4. 4.Potentially Hazardous Amine Absorber Pressure Vessels Used in Refinery Processing (standard interpretation memorandum) · US Occupational Safety and Health Administration (OSHA) ·
  5. 5.Research report on characterization and monitoring of cracking in wet H2S service (M. S. Cayard, R. D. Kane, L. Kaley, M. Prager), Welding Research Council Bulletin 396 (OSTI record 69967) · US Department of Energy, Office of Scientific and Technical Information (OSTI)
  6. 6.Research report on ultrasonic characterization and monitoring of cracking in wet H2S service (OSTI record 403561) · US Department of Energy, Office of Scientific and Technical Information (OSTI)
  7. 7.Comparative Analysis of Ultrasonic NDT Techniques for the Detection and Characterisation of Hydrogen-Induced Cracking (R. J. Kazys, L. Mazeika, V. Samaitis, R. Sliteris, P. Merck, Z. Viliunas), Materials 15(13):4551 · MDPI, via PubMed Central (open access, CC BY 4.0) ·
  8. 8.OSHA Technical Manual, Section IV, Chapter 2: Petroleum Refining Processes · US Occupational Safety and Health Administration (OSHA)