FactCorrosion and Damage Mechanisms · Environmental cracking

What is amine corrosion and amine cracking?

·7 sources

Short answer

Amine corrosion is metal loss in carbon steel amine treating units, driven mainly by dissolved acid gas and by contaminants such as heat-stable salts. Amine cracking is stress corrosion cracking of carbon steel in amine service, found mostly at welds that were not stress relieved. API RP 945 covers avoiding cracking in amine units.

By , Editor·Researched and drafted by ·Checked by , Editor·Last checked ·Next review

Why does it matter?

Amine alone does little to carbon steel; most of the damage comes from the acid gas it picks up and the contaminants that build up in it. Laboratory studies summarized by the US National Institute of Standards and Technology (NIST) found that pure amine did not crack carbon steel, while amine with carbon dioxide in the gas phase cracked it severely 1. A 2010 study likewise found steel stayed passive in an amine solution until carbon dioxide was added 5. In an industry survey of 294 amine plants summarized by OSHA, about 40% reported cracking 2.

Where does corrosion occur in an amine unit?

An amine unit removes hydrogen sulfide (H2S) and carbon dioxide (CO2) from gas or liquid hydrocarbons. The stream meets a counterflowing amine solution in an absorber (contactor), the loaded "rich" amine is stripped by heat in a regenerator, and the "lean" amine returns to the absorber 3. Common amines are monoethanolamine (MEA), diethanolamine (DEA) and methyldiethanolamine (MDEA) 3. Operating temperatures are typically about 38 to 93 °C (100 to 200 °F), so most equipment is carbon steel 2.

Plant experience reported in a 2010 study locates corrosion in four main places: the reboiler, the regenerator, the exchanger between rich and lean amine, and the lower part of the absorber. Attack can be uniform or localized, including pitting, erosion and stress cracking 5.

What drives amine corrosion?

  • Acid gas. Adding CO2 to an amine solution raised the corrosion rate of carbon steel and switched it from passive to active corrosion 5.
  • Type of amine. MEA gives a more corrosive solution than DEA, and MDEA is the least corrosive of the three; MEA and DEA form carbamates with CO2, which strongly affect corrosivity, while MDEA does not 5.
  • Heat-stable salts. Acids stronger than CO2, from feed contaminants or from amine breakdown, form salts that regeneration heat does not reverse. They lower the solution's pH and raise its conductivity, which promotes corrosion 5.
  • Temperature and oxygen. OSHA notes that regenerator bottom and reboiler temperatures need control to limit corrosion, and that oxygen must be kept out to prevent amine oxidation 3.

What is amine cracking?

Amine cracking is a form of stress corrosion cracking in carbon steel; NIST lists amine solutions among the environments known to cause it 1. In the survey of 294 plants, every crack was in or near a weld, most were in welds without post-weld heat treatment (PWHT), and cracking appeared in absorbers, regenerators, heat exchangers and piping 1,2. It occurred with several amines but was most frequent in MEA units 1,2. The roles of chlorides, cyanides and H2S were not fully understood when NIST reported in 1990 1.

API RP 945, Avoiding Environmental Cracking in Amine Units (4th edition, September 2022), gives guidance on carbon steel materials, fabrication, inspection and repair for these units 6.

How are amine corrosion and cracking found?

  • Cracking: wet fluorescent magnetic particle testing (WFMT) and ultrasonic testing were the main methods in the survey, with internal WFMT preferred 1,2.
  • Metal loss: ultrasonic testing measures general wall loss from the transit time of a sound pulse through the wall 2.
  • Repaired vessels: in the 1984 Romeoville, Illinois, absorber failure, magnetic particle testing revealed hundreds of cracks along welds and ultrasonic testing showed internal separation in the steel 7.

Where integrity problems show up

Where it occurs (unit or equipment)Conditions that drive itHow it is usually foundIn the Library
Absorbers, regenerators, heat exchangers and piping in carbon steelAmine with CO2; welds without PWHT; most often MEA units 1,2Internal WFMT, the preferred method, and ultrasonic testing 1,2What is stress corrosion cracking (SCC)?
Absorber bottom, rich-lean exchanger, regenerator and reboilerAcid gas loading, heat-stable salts, temperature 3,5Ultrasonic wall thickness measurement 2How does ultrasonic thickness measurement work?
Field-repaired absorbers and vesselsRepair welds not stress relieved; hard zones and hydrogen 4,7Magnetic particle testing for weld cracks; ultrasonic testing for internal separation 7What is wet hydrogen sulfide (H2S) damage?
Welds in new amine equipmentResidual stress and hardness left by welding 1Records of the type, extent and conditions of PWHT, which OSHA lists among data needed for safety assessment 2What is post-weld heat treatment (PWHT)?
Amine units capturing CO2 from flue gasOxygen-rich gas and sulfur oxides that form heat-stable salts 5Linear polarization resistance and weight-loss measurements, as used in laboratory studies of this service 5What is carbon capture and storage (CCS)?

Sources: NIST SP 780, 1990 1; OSHA Technical Manual, Section IV, Chapters 2 and 3 2,3; OSHA memorandum, 1986 4; Duan and others, 2010 5; NIST SP 958 7.

Common questions

Was the 1984 Romeoville absorber rupture caused by amine cracking?
Not primarily. OSHA's 1986 memo reported preliminary findings that unrelieved repair welds were especially sensitive to amine cracking, but NIST later stated that the full investigation found hydrogen-induced cracking, not amine cracking, was the primary cause. The failure still prompted the industry survey of amine units.
Is amine cracking the same as wet H2S cracking?
No. Amine cracking is stress corrosion cracking driven by the amine and CO2 environment at unrelieved welds. Wet H2S cracking comes from hydrogen produced by corrosion in water containing H2S; amine units can have both. See [What is an amine gas treating unit?](/library/amine-gas-treating/).
Which amine is most corrosive?
Of the three common amines, MEA gives the most corrosive solution and MDEA the least, and the survey found cracking most often in MEA units.

Beacon explains these concepts in its own words for education. It does not reproduce or replace the standards cited, and Winda is not affiliated with or endorsed by the organizations that publish them. Engineering decisions need the current edition of the standard and a qualified engineer.

Sources

  1. 1.NIST Special Publication 780, Guidelines for Pressure Vessel Safety Assessment (S. Yukawa) · US National Institute of Standards and Technology (NIST)
  2. 2.OSHA Technical Manual, Section IV, Chapter 3: Pressure Vessel Guidelines · US Occupational Safety and Health Administration (OSHA)
  3. 3.OSHA Technical Manual, Section IV, Chapter 2: Petroleum Refining Processes · US Occupational Safety and Health Administration (OSHA)
  4. 4.Potentially Hazardous Amine Absorber Pressure Vessels Used in Refinery Processing (standard interpretation memorandum) · US Occupational Safety and Health Administration (OSHA) ·
  5. 5.Effect of Oxygen and Heat Stable Salts on the Corrosion of Carbon Steel in MDEA-Based CO2 Capture Process (D. Duan, Y.-S. Choi, S. Nesic and others), NACE Corrosion 2010, Paper 10191 · NACE International; copy hosted by Ohio University, Institute for Corrosion and Multiphase Technology
  6. 6.2025 Publications Catalog (entry for RP 945) (RP 945, 4th edition, September 2022) · American Petroleum Institute (API)
  7. 7.Analysis of the Catastrophic Rupture of a Pressure Vessel (prepared by T. Siewert), in NIST SP 958, pp. 350-352 · US National Institute of Standards and Technology (NIST)