Skip to content
Beaconby Winda
FactCorrosion and Damage Mechanisms · Environmental cracking

What is caustic stress corrosion cracking?

·7 sources

Short answer

Caustic stress corrosion cracking, or caustic embrittlement, is cracking of carbon steel under tensile stress in hot sodium hydroxide (caustic) solutions. It is found mostly at welds and bends that were not stress relieved, and the cracks are fine, oxide-filled and mostly intergranular. API RP 571 covers it among refinery damage mechanisms.

By , Editor·Researched and drafted by ·Checked by , Editor·Last checked ·Next review

Why does it matter?

Continuous kraft pulp digesters run in a weak solution of a few percent sodium hydroxide and sodium sulfide at about 110 to 140 °C (230 to 285 °F), and for decades they had a good service record 1. After a digester ruptured suddenly in 1980, an inspection survey found some cracking in about 65% of the properly inspected vessels, and research traced it to caustic stress corrosion cracking (SCC), which was not expected at such low caustic strength 1,2. In refining, a 2023 case study describes two leaking welds in liquefied petroleum gas (LPG) piping exposed to small amounts of caustic carried over from treating 3.

What causes caustic SCC?

Like other forms of SCC, it needs three things together: a susceptible material condition, an aggressive environment and enough tensile stress; take any one away and the cracking does not occur 2. The US National Institute of Standards and Technology (NIST) lists hot or boiling caustic among the main cracking environments for carbon and low-alloy steels, which is where the old term "caustic embrittlement" comes from 2. The UK National Physical Laboratory gives carbon steel in hot alkaline solutions as a common example of SCC 7.

The stress is often residual. Hardness and residual stress in the heat-affected zone (HAZ) of welds without post-weld heat treatment (PWHT) make them susceptible 2, and the 2023 case study judged welding stress the likely driver at the leaking joints 3.

The bulk solution does not have to be strong. Caustic concentrates wherever water boils off and leaves solids behind: under deposits on boiler surfaces, in leaking riveted seams and along waterlines 4. In process piping, alternating wet and dry conditions and local overheating, for example from heat tracing, steam-out or temperature excursions, raise the risk 3. In the LPG case, outlet temperatures spiked to about 150 °C (300 °F) from a normal 60 °C (140 °F) 3.

Where does caustic SCC occur?

  • Boilers and steam systems. Caustic is a boiler water additive, and riveted drum boilers with leaking seams were the classic site of caustic embrittlement 4. Heat recovery steam generators are on the list too: cracks have turned up in the piping that carries their superheated steam 3.
  • Pulp digesters. All the digester cracking found in the survey was at welds 1.
  • Refinery caustic services. Refineries add caustic to desalting water and to desalted crude to cut chlorides, and use caustic washing to remove acids and sulfur compounds from hydrocarbon streams 5. Cracking appears where caustic is carried into hotter equipment, as in the LPG treating case 3.

What do the cracks look like and how are they found?

In the LPG welds, the cracks ran parallel to the weld in a web-like pattern, started at the inside surface, were filled with oxide and followed grain boundaries; they were found when a leak test revealed three leaks, then confirmed by wet fluorescent magnetic particle testing and metallography 3. In boilers the attack is intercrystalline cracking along grain boundaries 4.

For pulp digesters, wet fluorescent magnetic particle testing (WFMT) with proper surface preparation was the most effective detection method, and the guideline at the time was an annual examination 1. The US Occupational Safety and Health Administration (OSHA) summary of service cracking directs inspection toward welds and adjacent metal, and toward vessels never stress relieved or repaired without PWHT 1.

How is caustic SCC prevented?

  • Stress relief. PWHT of carbon steel welds and cold-formed bends is the usual mitigation, applied also to repair and attachment welds 3. Fully stress-relieved digesters were less susceptible 1.
  • Operating limits. The case study judged the LPG temperature spikes against limits in Association for Materials Protection and Performance (AMPP, formerly NACE) SP0403 and API RP 571 3; RP 571 (3rd edition, March 2020) covers more than 60 refinery damage mechanisms 6. Those limits are not reproduced here.
  • Material upgrade. For hotter or more concentrated caustic, nickel-based alloys can give better resistance 3.
  • Barriers. For digesters, weld cladding, spray coatings and anodic protection were studied 1.
  • Water treatment. In boilers, an inhibitor such as sodium nitrite dosed with the caustic, and avoiding waterlines and excess caustic, suppress the attack 4.

Where integrity problems show up

Where it occurs (unit or equipment)Conditions that drive itHow it is usually foundIn the Library
Continuous kraft pulp digestersA few percent caustic at 110 to 140 °C (230 to 285 °F); cracking at welds 1WFMT with good surface preparation; annual examination 1How are pressure vessels inspected?
Refinery LPG caustic treating and downstream pipingCaustic carryover concentrating in exchanger bypass piping; welds without PWHT 3Leak test, then wet fluorescent magnetic particle testing at welds 3What is post-weld heat treatment (PWHT)?
Caustic lines with heat tracing, or equipment steamed out after caustic serviceLocal overheating above the caustic service limit 3Temperature records, which showed the spikes in the LPG case 3What are integrity operating windows (IOWs)?
Carbon steel welds and bends in hot caustic without stress reliefResidual stress and hard heat-affected zones 2,3Inspection focused on welds and adjacent metal 1What are the main non-destructive testing (NDT) methods in oil and gas?
Boiler drums, seams and tubesCaustic concentrating at leaking seams, under deposits and at waterlines 4Grain-boundary cracks seen in sections of failed parts 4What is stress corrosion cracking (SCC)?

Sources: OSHA Technical Manual, Section IV, Chapter 3 1; NIST SP 780, 1990 2; AMPP Materials Performance, June 2023 3; KFUPM course notes 4.

Common questions

Is caustic embrittlement the same as caustic gouging?
No. Caustic gouging is metal loss in boiler tubes where concentrated sodium hydroxide dissolves the protective oxide, at deposits or along a waterline; caustic embrittlement is cracking.
Is caustic SCC the same as amine cracking?
They are related but separate. Both crack carbon steel at welds that were not stress relieved, but amine cracking occurs in amine units, and laboratory work cited by OSHA links it to amine with carbon dioxide present. See [What is amine corrosion and amine cracking?](/library/amine-corrosion/).
What material is used when carbon steel is not enough?
For higher temperatures or caustic concentrations, the 2023 case study points to nickel-based alloys for better resistance to caustic SCC.

Beacon explains these concepts in its own words for education. It does not reproduce or replace the standards cited, and Winda is not affiliated with or endorsed by the organizations that publish them. Engineering decisions need the current edition of the standard and a qualified engineer.

Sources

  1. 1.OSHA Technical Manual, Section IV, Chapter 3: Pressure Vessel Guidelines · US Occupational Safety and Health Administration (OSHA)
  2. 2.NIST Special Publication 780, Guidelines for Pressure Vessel Safety Assessment (S. Yukawa) · US National Institute of Standards and Technology (NIST)
  3. 3.Caustic SCC of Welded Fittings in LPG Service (S. Mahajanam), Materials Performance · Association for Materials Protection and Performance (AMPP)
  4. 4.Corrosion Engineering course notes, 4.10 Caustic Cracking · King Fahd University of Petroleum & Minerals (KFUPM), Department of Mechanical Engineering
  5. 5.OSHA Technical Manual, Section IV, Chapter 2: Petroleum Refining Processes · US Occupational Safety and Health Administration (OSHA)
  6. 6.2025 Publications Catalog (entry for RP 571) (RP 571, 3rd edition, March 2020) · American Petroleum Institute (API)