Skip to content
Beaconby Winda
FactCorrosion and Damage Mechanisms · Mechanical and metallurgical damage

What is temper embrittlement?

·6 sources

Short answer

Temper embrittlement is a loss of toughness in low-alloy steels, such as 2.25Cr-1Mo, after long exposure to, or slow cooling through, a range of roughly 320 to 525 °C. Impurities such as phosphorus, tin and antimony gather at grain boundaries. The steel keeps its strength but can break in a brittle way when it is cool.

By , Editor·Researched and drafted by ·Checked by , Editor·Last checked ·Next review

Why does it matter?

The loss therefore shows up when equipment is cool, not at operating temperature. For heavy wall chromium-molybdenum reactors in high-pressure hydrogen service, the American Petroleum Institute (API) has published technical reports since 2017 on setting a minimum pressurization temperature for start-ups and shutdowns of temper-embrittled 2.25Cr-1Mo steel in high-pressure hydrogen 4. Brittle fracture needs a crack-like flaw, high stress and low toughness together, so lost toughness makes any flaw more serious 5.

What happens inside the steel?

During long exposure in the embrittling range, impurity atoms move to the boundaries of the former austenite grains and weaken the bond between neighboring grains 1. The main embrittling elements are antimony, phosphorus, tin and arsenic; a 1977 review found antimony and tin the most effective, and noted that alloying elements encourage the impurities to segregate 1. In chromium-molybdenum steels without nickel, a 1980 technical report found phosphorus the main culprit, with manganese and silicon making it worse through their interaction with phosphorus 2. Grain boundary chemistry, grain size and hardness together set how far the transition temperature moves 2.

Sources give the damaging range differently: the 1977 review gives 320 to 525 °C 1, and a study published by API exposed chromium-molybdenum steels at 650 to 950 °F (343 to 510 °C) 3.

The damage can be undone: the 1977 review treats temper embrittlement as reversible 1, and the API-published study included repeated de-embrittlement of two embrittled steels 3.

Which equipment is at risk?

  • Heavy wall hydroprocessing reactors. API Publication 959 (1st edition, January 1982) characterized 64 commercial chromium-molybdenum steel samples, mostly 2.25Cr-1Mo, heat treated as for hydrotreater reactor fabrication; API notes that steel made up to about 1975 does not represent the low-susceptibility plate, forgings and weld metal generally available after 1975 4,3. API RP 934-A (3rd edition, January 2019) covers materials and fabrication of new heavy wall 2.25Cr and 3Cr steel vessels that will operate in hydrogen at high temperature and pressure 4. See What is hydroprocessing (hydrotreating and hydrocracking)?.
  • Steam turbine rotors. Chromium-molybdenum-vanadium rotors sampled after 15 to 26 years of service showed in-service temper embrittlement; phosphorus was the only residual element with a significant effect, and coarse grains raised susceptibility 6.

How is it tested and found?

  • Step cooling. A step-cooling heat treatment reveals susceptibility in the laboratory, and a 1989 study found it can simulate long-term service embrittlement except in very coarse-grained steel 6.

Where integrity problems show up

Where it occurs (unit or equipment)Conditions that drive itHow it is usually foundIn the Library
Heavy wall 2.25Cr-1Mo hydroprocessing reactorsYears in the embrittling range; impurity content of plate, forgings and weld metal 3,4Charpy tests on step-cooled or exposed samples 3What is hydroprocessing (hydrotreating and hydrocracking)?
Reactors at start-up and shutdownPressure applied while the embrittled steel is cool and holds dissolved hydrogen 4Not found by inspection; managed with minimum pressurization temperature limits, the subject of API's TR 934-F reports 4Minimum design metal temperature (MDMT)
Embrittled vessels with crack-like flawsFlaw, high stress and low toughness together 5Inspection for crack-like flaws; NIST notes flaws can sit in uninspected areas or be missed 5What are the main non-destructive testing (NDT) methods in oil and gas?
Steam turbine rotors (CrMoV)15 to 26 years in service; coarse grains 6Transition temperature shift measured on samples 6What is brittle fracture?

Sources: Shaw, 1981 3; API 2025 catalog 4; NIST SP 780, 1990 5; Cheruvu and Seth, 1989 6.

Common questions

Is temper embrittlement the same as hydrogen embrittlement?
No. Temper embrittlement comes from impurities gathering at grain boundaries during heat exposure. In hydroprocessing reactors the two interact, which is why API's TR 934-F reports study hydrogen-assisted cracking in temper-embrittled 2.25Cr-1Mo steel. See [What is hydrogen embrittlement?](/library/hydrogen-embrittlement/).
Can temper embrittlement be reversed?
Yes. The 1977 review describes it as reversible, and the API-published study examined repeated cycles of de-embrittlement.

Beacon explains these concepts in its own words for education. It does not reproduce or replace the standards cited, and Winda is not affiliated with or endorsed by the organizations that publish them. Engineering decisions need the current edition of the standard and a qualified engineer.

Sources

  1. 1.Reversible temper embrittlement (D. F. Stein), Annual Review of Materials Science 7 (record and abstract) · US DOE Office of Scientific and Technical Information (OSTI)
  2. 2.Elimination of impurity-induced embrittlement in steel. Part 1: impurity segregation and temper embrittlement (C. J. McMahon Jr. and others), technical report (record and abstract) · US DOE Office of Scientific and Technical Information (OSTI)
  3. 3.Characterization study of temper embrittlement of chromium-molybdenum steels (B. J. Shaw), Proceedings, API Refining Department, vol. 60 (record and abstract) · US DOE Office of Scientific and Technical Information (OSTI)
  4. 4.2025 Publications Catalog (entries for Publ 959, RP 934-A and TR 934-F, Part 1) (Publ 959, 1st edition, January 1982; RP 934-A, 3rd edition, January 2019; TR 934-F, Part 1, 1st edition, 2017) · American Petroleum Institute (API)
  5. 5.NIST Special Publication 780, Guidelines for Pressure Vessel Safety Assessment (S. Yukawa) · US National Institute of Standards and Technology (NIST)
  6. 6.The influences of impurity content, tensile strength, and grain size on in-service temper embrittlement of CrMoV steels (N. S. Cheruvu, B. B. Seth), Metallurgical Transactions A 20A (record and abstract) · US DOE Office of Scientific and Technical Information (OSTI)