Skip to content
Beaconby Winda
FactCorrosion and Damage Mechanisms · Corrosion control

How are biocides used to control microbiologically influenced corrosion?

·11 sources

Short answer

Biocides are chemicals that kill or suppress the microorganisms behind microbiologically influenced corrosion (MIC) in water-bearing oil and gas systems. Oxidizing and non-oxidizing types are dosed into the fluid, often alongside mechanical cleaning and monitoring. In the US, such products must be registered as pesticides with the Environmental Protection Agency (40 CFR 152.15).

By , Editor·Researched and drafted by ·Checked by , Editor·Last checked ·Next review

Why does it matter?

As molecular testing spread, asset owners found microorganisms almost everywhere in their systems, but cell counts correlated poorly with actual MIC damage, according to a 2023 review 2. The same review notes that microbes living in a biofilm on the wall can tolerate treatment far better than free-floating cells, in an extreme case about 1,000 times better 2. A biocide program therefore has to be judged by what happens at the metal surface, not only by bacteria counts in a water sample 2.

How do biocides control MIC?

MIC is corrosion accelerated by microorganisms and their products, which mostly live in biofilms: layers of cells held together by a slime of sugars, proteins and other substances they secrete 1. The corrosion glossary of the UK National Physical Laboratory (NPL) defines a biocide simply as an added chemical whose job is to kill living things 11. Biocides attack cell membranes and enzymes, killing the microbes and breaking down biofilm 1. A 2023 review by Shi and co-authors describes them as the most cost-effective MIC control in practice 1.

They are one option among several. Knisz and co-authors list biocides alongside corrosion inhibitors, oxygen scavengers, flow velocity control, pigging or flushing, ultraviolet treatment, separators and filters, and control of fluid quality 2. In some oilfields, nitrate is added so that nitrate-reducing bacteria outcompete the sulfate-reducing bacteria that produce hydrogen sulfide (H2S) 1,2. Corrosion inhibitors on their own do not control MIC: the UK Health and Safety Executive (HSE) finds them ineffective against it 3.

Which biocides are used?

ClassGeneric examplesHow it actsLimits reported
OxidizingChlorine, sodium hypochlorite, chlorine dioxide, bromine compounds, ozone, hydrogen peroxideOxidizes membranes, enzymes and biofilm materialReacts with organic matter, so the effect is unstable; excess can raise metal corrosion; little effect on biofilm formation
AldehydesGlutaraldehyde (the most common)Enters cells and binds proteinsToxic
Quaternary ammonium compoundsSingle, twin-headed and polymeric formsPositive charge binds the cell wall and damages the membrane; some also inhibit corrosionLong use can breed resistance
Quaternary phosphonium saltsTetrakis(hydroxymethyl)phosphonium sulfate (THPS), the most common in oilfieldsSimilar to quaternary ammoniumToo low a dose can stimulate growth in the biofilm
Heterocyclic compoundsIsothiazolinonesBlock the cell's energy supply and damage DNAReact with H2S, so unsuitable for sulfide-bearing injection water; low doses can increase growth
Organobromine compoundsNon-oxidizing bromine-containing biocidesEfficient, broad-spectrum killingSome breakdown products are more toxic or persistent than the parent

Source: Shi et al., 2023 1. Generic chemical classes only; no products or suppliers are named.

How are biocides applied?

  • Continuously or repeatedly. Industrial systems keep receiving new microbes, so a single treatment cannot eradicate them and control requires continuing doses 1.
  • At an effective dose. Cells in biofilms need higher concentrations than free cells, and doses that are too low can stimulate growth 1.
  • Varied over time. Using the same biocide for a long time promotes resistance and rising doses, and excess use can cause scaling 1. Mixing biocides, or adding enhancers such as chelating agents or D-amino acids, can lower the dose needed 1.
  • With cleaning. Pigging and flushing remove biofilm and deposits but do not stop regrowth; in seawater a biofilm can form within minutes 2. Mechanical cleaning can also spread microbes from damaged biofilm, so it is often paired with chemicals 1.

In the US, a product intended to protect industrial processes, systems or water from fouling or deterioration caused by bacteria and other microbes is an antimicrobial pesticide 5, and no one may distribute or sell a pesticide that is not registered under the Federal Insecticide, Fungicide, and Rodenticide Act (FIFRA) (40 CFR 152.15) 6. The Environmental Protection Agency (EPA) groups cooling tower and jet fuel treatments among non-public-health antimicrobial uses 4. In the European Union, coatings that release biocides are regulated under the Biocides Regulation 2.

How is a biocide program judged to work?

Knisz and co-authors describe corrosion management as a repeating cycle of threat assessment, mitigation and monitoring, in which microbiological data are read together with coupons, probes, inspection results, operating conditions and fluid chemistry 2. No single test proves MIC, so investigators combine multiple lines of evidence 2. Molecular microbiological methods help show whether a new treatment changes the types, numbers and activity of microbes where corrosion occurs, but collecting biofilm samples from a working asset and analyzing them before genetic information degrades is a main practical difficulty 2. Where nitrate is injected, sulfate, sulfide, nitrate and nitrite are monitored closely to set doses 2.

Where integrity problems show up

Where it occurs (unit or equipment)Conditions that drive itHow it is usually foundIn the Library
Low point downstream of a partly clogged drip 7Microbes with water, chlorides, oxygen, carbon dioxide and H2S; liquids bypassed the drip and cleaning pigs could not run 7Microbial tests of deposits from scrubbers, drips and pig receivers; coupons and in-line inspection 7What is microbiologically influenced corrosion (MIC)?
Dead legs and piping with no flow or stratified flowWater and solids settle and biofilms grow 2Design and operating records reviewed to find such areas and target inspection 2Dead leg
Deposits and biofilm in water-handling linesSessile cells tolerate biocide; low doses can stimulate growth 1,2Coupons and probes with biofilm sampling and molecular methods 2What is under-deposit corrosion?
Buried pipe in waterlogged, airless claySulfate-reducing bacteria active without oxygen 8; NPL calls for a more negative cathodic protection potential on steel where they are present 9On excavation, black product smelling of H2S over a shiny surface; tests for anaerobic or corrosion-accelerating bacteria 8,10What is soil corrosion?

Sources: NTSB PAR-03/01 7; Knisz et al., 2023 2; Shi et al., 2023 1; NPL Guide No. 4 8; 49 CFR 192.455 10.

Common questions

Is a biocide the same as a corrosion inhibitor?
No. NPL defines a biocide as an additive that kills living organisms, while an inhibitor slows the corrosion reaction at the metal; HSE finds inhibitors ineffective against MIC. Some quaternary ammonium biocides also inhibit corrosion, so one product can do both jobs.
Can pigging alone control MIC?
No. Knisz and co-authors note that mechanical cleaning removes biofilm but does not prevent it re-forming, so it is combined with chemical treatment.
How is MIC on the outside of a buried pipe controlled?
Mainly with coatings and cathodic protection. NPL gives a more negative protection potential for steel where sulfate-reducing bacteria are active, and Knisz and co-authors note that field reports support cathodic protection against MIC while laboratory evidence is less certain.

Beacon explains these concepts in its own words for education. It does not reproduce or replace the standards cited, and Winda is not affiliated with or endorsed by the organizations that publish them. Engineering decisions need the current edition of the standard and a qualified engineer.

Sources

  1. 1.Comprehensive Review on the Use of Biocides in Microbiologically Influenced Corrosion (X. Shi, R. Zhang, W. Sand and others), Microorganisms 11(9):2194 · MDPI (open access, CC BY 4.0) ·
  2. 2.Microbiologically influenced corrosion: more than just microorganisms (J. Knisz, R. Eckert, L. M. Gieg and others), FEMS Microbiology Reviews 47(5):fuad041 · Oxford University Press on behalf of FEMS (open access, CC BY 4.0)
  3. 3.RR1023: Reliable corrosion inhibition in the oil and gas industry (J. Hobbs, Health and Safety Laboratory, 2014; archived copy, withdrawn from hse.gov.uk) · UK Health and Safety Executive (HSE)
  4. 4.What are Antimicrobial Pesticides? · US Environmental Protection Agency (EPA)
  5. 5.Antimicrobial Pesticide Registration · US Environmental Protection Agency (EPA)
  6. 6.40 CFR 152.15, Pesticide products required to be registered (with 152.3 definitions) · eCFR, US Office of the Federal Register
  7. 7.Pipeline Accident Report NTSB/PAR-03/01: Natural Gas Pipeline Rupture and Fire Near Carlsbad, New Mexico, August 19, 2000 · US National Transportation Safety Board (NTSB)
  8. 8.Guides to Good Practice in Corrosion Control No. 4: Corrosion Control for Buried Pipelines (D. W. Harvey) · National Physical Laboratory (NPL), UK
  9. 9.Guides to Good Practice in Corrosion Control No. 1: Cathodic Protection (D. W. Harvey) · National Physical Laboratory (NPL), UK
  10. 10.49 CFR 192.455, External corrosion control: Buried or submerged pipelines installed after July 31, 1971 (Part 192, Subpart I) · eCFR, US Office of the Federal Register
  11. 11.Guides to Good Practice in Corrosion Control No. 11: Corrosion control checklist · National Physical Laboratory (NPL), UK